The question you ask is a bit bigger that i think you expect, but basically, nylon normally has a low melt viscosity and a very sudden transition from solid to liquid. Amorphous nylons tend to be less sudden.
Also nylon is hygroscopic, and if it has absorbed much water, then the outguessing as the water boils off will force some material out the nozzle as drool. If it is moisture causing the drool, the drool will spit and bubble with gas (steam) discharging from the melt.
Bottom line answer.
Ensure the granules are dry.
Ensure the nozzle heater is in good condition, is in good contact with the nozzle (good clean smooth mating surface).
Ensure the heater is very close to the tip of the nozzle.
Use a variable voltage controller to the nozzle, NOT AN ON OFF cycling type controller. DME controllers or even domestic light dimmer switches all work OK.
The temperature fluctuation during reaction times with on off type controllers is enough to cause drool then freeze then drool then freeze cycles to be set up.
Regards
pat pprimmer@acay.com.au