Flat-rolled stainless producers shot blast hot-rolled stainless plate and sheet coils before pickling to loosen the embedded-type scale which is hard to pickle off. What do bar producers do to break up the hot mill scale before anneal and pickle?

Michael McGuire
 
Replies continue below

Recommended for you

ASM HANDBOOK Volume 1 describes several conditions for stainless steel bar finishing:

Hot worked only: [1] scale not removed (except for spot conditioning), [2] rough turned, [3] blast cleaned

Annealed or otherwise heat treated: [1] scale not removed, [2] rough turned, [3] pickled or blast cleaned & pickled, [4] cold drawn or cold rolled, [5] centerless ground, [6] polished

Carpenter mills the surface of larger section square bars in order to remove the scale from hot-rolling.
 