Situation: Concrete post-tensioned beams poured on top of bridge piers. These post-tensioned beams will carry concrete slab that will be deck asphalted for future traffic. During one pour of 300 cubic meters for around 20 such beams, 1 beam web showed delayed concrete setting. This one beam was monitored for setting day-by-day using Schmidt hammer. The results of Schmidt were improving every day so everyone wanted to wait and watch until 14 days. So at the end of 14 days all the concrete surface was hard and Schmidt readings were average 34 except few areas half meter by half meter where it was only 24. There are also random cracks mostly of horizontal nature along the length of the beam web.
The web beam is 500mm thick x 1700mm high x 13 meter long. Post tensioned cables are running along the length of the beam with 100mm cable cover to concrete.
Cores were obtained from the affected areas of concrete due to late setting. The percentage strength achieved in cores is 54% on average of the design strength of 45 Mpa. The age of core at testing is 21 days.
The consultant's demand repair with epoxy injection for strengthening the beam before post-tensioning and undertaking responsibility for the integrity of the structure.
Based on the above info what are the vulnerabilities from structural point of view and stability of the beam during post-tensioning and service period noting that heavy highway traffic loads are expected on this bridge.
attached photo of the web beam.
Thanks in advance
Situation: Concrete post-tensioned beams poured on top of bridge piers. These post-tensioned beams will carry concrete slab that will be deck asphalted for future traffic. During one pour of 300 cubic meters for around 20 such beams, 1 beam web showed delayed concrete setting. This one beam was monitored for setting day-by-day using Schmidt hammer. The results of Schmidt were improving every day so everyone wanted to wait and watch until 14 days. So at the end of 14 days all the concrete surface was hard and Schmidt readings were average 34 except few areas half meter by half meter where it was only 24. There are also random cracks mostly of horizontal nature along the length of the beam web.
The web beam is 500mm thick x 1700mm high x 13 meter long. Post tensioned cables are running along the length of the beam with 100mm cable cover to concrete.
Cores were obtained from the affected areas of concrete due to late setting. The percentage strength achieved in cores is 54% on average of the design strength of 45 Mpa. The age of core at testing is 21 days.
The consultant's demand repair with epoxy injection for strengthening the beam before post-tensioning and undertaking responsibility for the integrity of the structure.
Based on the above info what are the vulnerabilities from structural point of view and stability of the beam during post-tensioning and service period noting that heavy highway traffic loads are expected on this bridge.
attached photo of the web beam.