Hi experts,
Could you please share your experience regarding CVN impact testing for ER70S-6 filler metal?
I’m currently qualifying a PQR for A333 Gr.6 to API 5L Gr.X65 using ER70S-6 (GTAW + SMAW).
When conducting the weld metal impact test (full-size specimens) at -46 C degree, I obtained very inconsistent results: 11 J, 120 J, and 80 J.
I repeated the test on another set of CVN specimens, but the same pattern appeared — two high values and one significantly low value.
All three specimens were taken from the same area of the weld on a test coupon (pipe 6" OD, 11 mm thickness).

I’m trying to understand the cause of this variation.
Has anyone encountered this issue before? Any insights or suggestions would be greatly appreciated.

Thanks in advance!
 
Replies continue below

Recommended for you

There are many errors during specimen extraction, machining, and testing.
Did you witness all the steps?.
 
Were the notches ground or broached?
I loathe broached notches.
 
And the impact test at the HAZ?

Was another test performed?
 
So you also looked at the face of the notch to assure that there was no tearing or chatter?
 
So you also looked at the face of the notch to assure that there was no tearing or chatter?
I am sure that no tearing or chatter at the notch.
Yesterday, I changed the CVN test to another test lab.
At the first set, results of absorbed energy are 12J, 43J, 85J.
The second set, results are 53J, 33J, 28J.
The CVN results of ER70S-6 in certficate are 151J, 153J, 147J in 1G position.
It is very difficult for me to explain the test results to Client.
 
And the impact test at the HAZ?

Was another test performed?
No sir. It is tested at weld metal.
Another test performed at other test lab. Please see my response above.
 
The consumable batch certificate is 3.1 or 2.2 ?
 
@Karik87
You said: "It is very difficult for me to explain the test results to Client."

Well, you need to read more and take a welding and NDT training course
Impact test requires a step-by-step inspection by qualified personnel.
 
Last edited:
@Karik87
You said: "It is very difficult for me to explain the test results to Client."

Well, you need to read more and take a welding and NDT training course
Impact test requires a step-by-step inspection by qualified personnel.
r6155,
Stop being so bloody critical all the time.
You do nothing on this forum but criticise.
"It is very difficult for me to explain the test results to Client." - do you with all your wisdom have an explanation to offer the Client ?
karik87 does not need to be qualified or to take a Welding or NDT training course - the test laboratories are required to be certified with qualified personnel.
He has chosen to take the samples to a 2nd laboratory and there are still issues.
Steve Jones has given a very valid response - how accurate is the consumable batch certificate ?
 
I've seen these type of results numerous times. Most often a result of notch location (weld dilution) and notch machining.
 
The consumable batch certificate is 3.1 or 2.2 ?
The consumable certificate is 3.1 with CVN results as 151J, 153J, 147J in 1G position, Sir.
 
Last edited:
I've seen these type of results numerous times. Most often a result of notch location (weld dilution) and notch machining.
This is the 1st time I have seen inconsistent results of CVN tests.
As you see the below photo, the notch location is in the middle of weld metal.
5.jpg

@SJones @DekDee @EdStainless @weldstan Thank you very much for taking the time to share your valuable opinions. Based on the discussion, I believe that the consumable batch certificate may not be fully accurate.
 