Does anyone know where I can get compressive creep data for Nylon 6 (not Nylon 6, 6)? I am looking for data going out to 3 years at least or some way of parametrically (e.g. Larson Miller Parameter) extrapolating/interpolating the creep strain to 3 years.
 
I am pretty sure I have some data in an old archive. I know I have plenty for 6.6, but I think also a lesser amount for type 6.

What temperature and load.

I presume Std injection moulding grade with lube and nucleating agents moisture conditioned to equilibrium at 23 deg C at 50% humidity. Degree of crystallinity is an important variable.

Regards
Pat
See FAQ731-376 for tips on use of eng-tips by professional engineers &
for site rules
 
Hi Pat,

We purchased to ASTM D5989 Type 2 (They call it type 6, but I believe they mean Nylon 6 because they refer to the cast/compression molded version). Room temperature, 7ksi. If you have equivalent for compression molded Nylon 6,6 I could use that too. If properties are better than Nylon 6, I might recommend that instead. Sorry, don't know degree of crystallinity. I'll take what you have at this point.
 
The terms nylon type 6 and nylon 6 are used interchangeably.

Degree of crystallinity varies by grade, moulding conditions and colours used. The grade and conditions are noted on test results. I am just saying there is a good chance that your mouldings will perform different to the test specimens.

I only have data for injection mouldings

Regards
Pat
See FAQ731-376 for tips on use of eng-tips by professional engineers &
for site rules
 
Anyone have isochronous data for nylon 6? I can make use of that.
 
I just found some data.

Isochronous stress vs strain for Maranyl Nylon 6 for both controlled crystallinity (nucleated) grade and unmodified grade (basically barefoot resin with minimal mould release lubricant).

Performed over 100 seconds 20 deg C dry specimens.

Horizontal axis is %age strain starting 0.1% strain and finishing 2% strain logarithmic scale.

Vertical axis is stress in psi starting 3 and finishing 10,000

Results are straight lines

First line is unmodified grade starting bottom left at 3.9psi & 0.1% strain & finishing top right 6,000psi & 1.7% strain.

Second line is nucleated grade starting bottom left at 4.2psi & 0.1% strain & finishing top right 6,900psi & 1.7% strain.


Regards
Pat
See FAQ731-376 for tips on use of eng-tips by professional engineers &
for site rules
 
Thanks Pat, That helps a little.
Anything for at least a thousand hours?
 

If you go here: DSM, click "Material Selector" on right, look down for Akulon K222D (unfilled PA6), click underlined link>properties>Fct on tabs>take your pick of graphs.

Cheers

Harry



www.tynevalleyplastics.co.uk

It's ok to soar like an eagle, but weasels don't get sucked into jet engines.
 
Pud,

what does the "cond" modifier mean?
 
Cond means moisture conditioned according to a specification that should be noted. Probably 50% RH at 23 Deg C as opposed to dry as moulded. It makes a VERY substantial difference. It is also typical of the average real world, but not representative of the extremes in the real world.