We are building a clad pressure vessel and the customer wants us to do a copper sulfate test where the clad surface has been removed for weld prep to check for clean base metal. Does anyone have a procedure or information on the procees to do this.
 
Replies continue below

Recommended for you

remove the clad

wire brush to remove all stainless

spray on the copper sulphate

all carbon steel surfaces should turn orange

 
should have added

any stainless steel surfaces still bonded to carbon steel will not change colors.

what you will be looking for is areas that do not change colors

the test is to verify all stainless has been removed 3/8" to 3/4" away from the weld surfaces

after welding and clearing all carbon steel NDE, you will do a clad restoration weld (overlay) and do nde on the stainless welding
 
Thanks for the reply. This is exactly what I thought but what I want to know is what strength to mix the copper sulfate. I found it in 50 lb bags and was told to mix it with distilled water but I do not know the strength. If I mix it too strong will the residue do damage. I have also read that for some applications there is sufuric acid in the mix as well?
 