Spinda,
at 1000 deg C tradtional composite materials will not work. Even more advanced resin systems such as polyimide or BMI have Tg's of only 400 Deg C. But, you may be able to use Carbon-Carbon composites which have the resin burned off and infiltrated with carbon. C-C can maintain strengths of 250 to 400 Mpa up to temperatures of 1800 deg C. But, due to the fibers and matrix having higher thermal conductivties, C-C has typical in-plane k values of 50 W/mK for Pan fibers and up to 250 W/Mk for pitch based fibers. But, thru thickness and across ply are usually less than 5 W/mk. Hope this helps and good luck,
J-Mo