C360 Half Hard Brass is what is on the print. We got in C36000 Cast and Turned. I was able to find info on C36000 but haven't been able to find anything on C360 Half Hard. Can anyone provide me with the specs on C360 Half Hard?

Thank You.


 
Replies continue below

Recommended for you

Typical mechanical properties for alloy C36000 in the H02 (half-hard) condition are as follows:

diameter tensile strength yield strength elongation HRB shear strength

6 mm (0.25") 470 MPa (68 ksi) 360 MPa (52 ksi) 18% 80 260 MPa (38 ksi)

25 mm (1") 400 MPa (58 ksi) 310 MPa (45 ksi) 25% 78 235 MPa (34 ksi)

50 mm (2") 380 MPa (55 ksi) 305 MPa (44 ksi) 32% 75 220 MPa (32 ksi)
 
Thank you, TVP. I appreciate your expertise.

I have contacted our vendor. (What I should have done in the first place.) He informed me that our part was too large to be half hard and parts this size are 'as cast'. How much does the material properties of brass vary in the 'as cast' state? The info I've gathered isn't too promising; the yield strength for C36000 can vary between 124 and 340 Mpa.

 