Currently, we are using chromium-copper for electrodes in our projection welding processes. Due to several "Quality" isssues, a question has arised about using beryllium-copper, instead. I understand that this is a more durable material, but could the lower conductivity of the beryllium-copper cause issue? Can anyone provide info on a comparison of the 2 materials.

Thank you.
 
I can't give a definite answer (probably depends upon cycle & weld material parameters), but it seems worth testing the beryllium copper. For maximum conductivity, try the ‘low beryllium’ C17500 alloy in the fully age hardened condition. Possibly, a brief delay prior to applying current to lose some heat to the workpiece would allow use of a harder Be copper alloy. Some material parameters:

Material Alloy YS, MPa Hard.,HV %IACS Thermal cond.
0.7%Cr C18500 530 125 80-85 324 W/m-K
low Be C17500 650-870 230 45-52 200 W/m-K
Be copper C17200,C17400 965-1340 360-420 22-25 105-130 W/m-K
cast “ “ C82400 965 367 18 100 est.

Notes: Properties for all alloys in precipitation hardened condition.
The 0.8%Cr C18400 alloy has approximately the same values as C18500.
‘low Be’ is 99.6Cu-0.6Be-2.5Co in HT (TH04) Temper.
Data are from MatWeb.com, ‘Copper and Copper Alloys: Compositions and Mechanical Properties,’ CDA No. 36, 12th Edn., London (1964), and Metals Handbook, Vol. 2, 8th Edn., ASM, Metals Park, OH (1964).

Please report any results.
 
Thanks for the information...and the reply
 