I am looking for a way to remove mild steel from a nitronic 40 piece. The steel was used as a filler during a spraying process. From what I can gather, HCL may be a suitable solution. I have found that it should be less than 1% to not attack the notronic 40. Will that be strong enought to aggressively attack the steel?
 
Replies continue below

Recommended for you

Try using an acid which passivates stainless and dissolves carbon steel like hot, dilute HNO3. 5-10% and over 50C.
 
I ended up trying many things and, for my application, 33% Acetic acid above 80C worked the best. Believe it or not.
 
That's very interesting that acetic could do the job. I appreciate the feedback.
 