Dear All,
During my review of an material test certificate of A516 Gr70 plate material,the supplier has qualified the UT testing of a plate to level B. I raised a query of why not qualified for level C, which is the stringent one and as required by ASTM A20 requirement also. However received an response from supplier that the applicability of ASTM A20 shall apply only to non heat treated plates and or plates only with stress relieving, as indicated on section 1.4 of A516.
Is ASTM A20 not applicable for heat treated or normalized material. Please confirm.
 
Replies continue below

Recommended for you

My query is all about the interpretation of section 1.4.. my understanding on this section,is that the normalized plated or heat treated plates wouldn’t be tested or complying to general requirements in accordance with ASTM A20?? If so, how to determine the UT acceptance level for a material or the subsequent testing applications?
 
Did you invoke Supplementary testing for UT in SA 516 S8 or S12?
 
Besides the supp. testing, the only reference I see in A-20 in regards to UT is 5.37. This is applicable to strand casting.
 
I don't have the latest versions at hand but:

SA-516, 1.4 refers to plate produced from coil and furnished w/o heat treat or with stress relief only. I don't see that SA-516 or SA-20 either one requires UT for any plate condition. If UT per SA-578 is performed, the purchase shall specify the acceptance level.

Looks like the supplier UT'd even though not required, and picked the acceptance level.

Regards,

Mike

The problem with sloppy work is that the supply FAR EXCEEDS the demand
 
Hi mike, as far as my understanding.. all ASTM A516 plate materials shall be UT tested in accordance with A578 for identification of discontinuity or cracks in the plate material.
If ASTM A20 is not applicable for heat treated plates ( normalized) [pre][/pre]as indicated in section 1.4, then my question is how to determine the level of acceptance criteria (A, B or C) as per A578??
 
516 plates do not require UT....where are you getting this information?
 
ET1983, your understanding is not correct. Except for strand-cast plates, as per david339933 UT is not required by either SA-20 or SA-516, including 1.4.

UT and acceptance criteria is only as specified by the buyer.

You need to carefully read both specifications.

Regards,

Mike

The problem with sloppy work is that the supply FAR EXCEEDS the demand
 
Completely agree with SnTMan & david339933.
But I guess ET1983 requires a little more clarification.
UT is specified for non-heat treated and/or stress relieved steels as there could be cold cracks during or after cold rolling.
However, normalization is done during hot rolling, thereby enhancing the toughness of the steel. Cold cracking is not envisaged and hence the code does not ask for UT.
 