Not quite, yield stress = f(Temperature and time @ Temperature).
From MIL-HDBK-5J,
Figure 3.2.3.1.1(b). Effect of temperature on the tensile yield strength(Fty) of 2024-T3, T351, and 2024-T4 aluminum alloy (all products except extrusions).
[Curves are shown for 1/2, 10, 100, 1000 & 10,000 hours.]
At 400oF, yield strength as % of room T value:
1/2 hr 78%
10 76
100 70
1000 60
10,000 46
Note: these values are more accurate than in previous post where I read off monitor; these are from a printout.