Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations KootK on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Aluminum Weld Shear Strength?

Status
Not open for further replies.

PhilipFry

Mechanical
Aug 3, 2001
56
Here's an easy question. I'm using 4043 to weld two 6061-T6 tubes and I'm trying to figure out the strength of the weld. I've found some literature that says the minimum shear strength of a weld using 4043 is 15 ksi. Does that figure include the weld efficiency, or would I need to knock that number down even further?
 
Replies continue below

Recommended for you

No, I would believe that the ultimate shear strength number that you stated is a measured value of the weld metal. Not exactly sure what you mean by weld efficiency, but if you are going to use this strength value you might want to assign a reduction factor for design margin. What type of weld joint design are you going to use - a fillet or full penetration weld to join the tubes?
 
6061-T6 welded with ER4043, non HT the yield strenght welded is reduced to 18 KSI, Ultimate tensile welded is ~27 KSI. Typical shear is 60% of yield. The weld eff will also reduce the allowable load further.

Consider a full pent weld and HT if full strength is required.
 
From the little ALCOA Handbook:
Welded butt joints.
Minimum expected strength. (Called design point by ALCOA)
Welded with no post weld heat treatment.

6061-T6 welded with 4043 under 3/16" thick:
UTS 24,000 psi YS 20,000 psi

6061-T6 welded with 4043 over 3/16" thick
UTS 24,000 psi YS 15,000 psi

::

Minimum Shear Strength of 4043 Filet Weld after naturally aging 2-3 months.

Shear Strength 11,500 psi

 