I'm looking for the following data for A14130 (A413.0):-

Elastic modulus
Shear modulus
Compressive strength
And
Thermal expansion coefficient


Also what is the difference between LM24 and A413.0?

Thanks in advance
 
Yes.
But I can't find the above info there.
And there is no reference to LM24 on the site.

You say the shear modulus is about 27 GPa. How accurate is that?
 
The ASM Handbook Series lists the elastic modulus (E) of this alloy as 71 GPa and Poisson's ratio ([ν]) as 0.33. That results in a Shear Modulus (G) of 27 GPa according to the equation G = E/[2(1+[ν])]. The Matweb link above lists the thermal expansion coefficient and strength (you can assume tension and compression are equal).


Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Thanks for the help.
But please excuse my ignorance, where dose the link above give me the thermal expansion coefficient?
 
Towards the bottom, there is a property listed as "CTE, linear 20°C". This is the Coefficient of Thermal Expansion.

Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 