Hi Googbadgood,
Failures in HIC testing are lot attributed to the manufacturing and the cleanliness of the steel.Welding comes next.
APL-5L-Annex H specifies many quality requirements some of which are as follows:=
H.3.2 Steel making:-The steel shall be made to a clean steel practice, by either the basic oxygen steel-making process or the electric furnace process & shall be killed.
--Vacuum degassing or alternative processes to be used to reduce the gas content.
--The molten steel shall be treated for inclusion shape control.
--A procedure (e.g. metallographic examination) may be agreed between the purchaser and the manufacturer to assess the effectiveness of inclusion shape control.
--For S levels ≤ 0.001%, inclusion shape control may be waived by agreement.
H.4.3 HIC/SWC test to be met.
Were all these requirements met at the first place.
What were the requirements of the P.O.
Appreciate your response.
Thanks.
Pradip Goswami,P.Eng.IWE
Welding & Metallurgical Specialist
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299
All provided answer are personal opinions or personal judgements only. It's not connected with any employers by any means.