We are using a M10 locknut. The material is "A2" and the locking mechanism is a nylon ring at the end of the thread. Commonly called a "Nylock" in our area.

The make thread that it is going on is 303 Stainless.

Issue: severe gauling/seizing when we engage the locking mechanism.

Question: What would be the best grade of SS for the locknut to reduce gauling? I don't think I can change the 303 on the male thread.
 
- try slowing down the wrench speed. Don't use the nut to "take up" the joint, and minimize thread protrusion past the nut as much as possible.

- lubricate the threads with a good anti-seize

- yes, you can try a different grade of stainless nut material, if you can find it, but unless you can get nuts made from a gall-resistant alloy (gall tuff, nitronic ...) your results may vary. If you switch to a standard grade 5 alloy nut (i.e. steel, not stainless) it probably will never gall. You can get those in zinc plated versions...
 
Try A4 (316) Stainless. It is less prone to galling than A2 (304).
Hand tighten, don't over torque - and once installed it should not be taken on and off regularly without an anti seize. Unfortunately, 303 isn't as anti galling as 316 - too bad you are stuck with the thread.

good luck
 
Are the threads rolled? This is often a more serious issue with cut threads.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 
Ed, these are NOT rolled. The male thread is cut on a lathe....
 