Magnetrics,
probably it depends on mine and your poor english but I need to clarify some subjects
1)I'm only a old metallurgical technician and I have never sold steel. Therefore,I'm not a commercial guy.
2)I don't understand if you must use the 15.5PH or 440C that you have in your yard or if you can buy different grades if these ones were available in your country or in other one.In both cases, your problem is the small quantity because neither Cartech nor other steelmaker wants to supply. Am I right ?
3)You said you are in contact with the Authors of paper. I hope they will give you some help because, usually, this Steelmaker is habit to supply information about his grades.Waiting for these data , I seem you could find some first info also from the paper. Particularly, you can verify magnetic permeability reach the maximum ( from 100 to 150 approx ) at H1025 (550°C)at any value of Cr/Ni eq.
Moreover , you can verify Jsat is between 1,3 and 1,6 T ( for 15.5PH you have to consider close to 1,3 than 1,6T)
4) If you are forced to use the 15.5PH, the first thing to do is:
a)to verify the certificate of the Steelmaker: which condition? If cond A,you can do a aging at temperature you prefere remembering that the maximum permeabilty will be reached at H1025 ( 550°C)
b)From the chemical analysis of certificate, you could foresee the values of mag.perm. by Cr/Nieq.
5) About 440 C, I have some data but I need to know if you want to use as annealed or as H+T . In this last case, mag.perm will depend on amount of retained austenite and Hrc. However , in both cases , Mag.perm = 65- 100.
Annealed condition is higher but this grade is not use in this condition.
Finally, if you decide to find and buy different steel grade, there is a large choice but it's mandatory to understand if you want stainless steel and its mechanical properties. Otherwise, we will continue to discuss whithout conclusion.
And if the Authors gave an answer, you could ask them if they could supply other data for different grades.
Let me know. Probably you are lucky !