What is the maximum ppm of chlorides that a 316L stainless steel can withstand? What about the temperature effects?

I searched the internet and saw 1000 ppm but also one which said 3-5 ppm.

Can anyone let me know about this?

Thanks in advance
 
You will get as many answers as there are people on this Forum.
Can you come back with a little more of the conditions that you are considering for the exposure. Things like the enviroment, stess levels, and such.
 
unclesyd:
I am not very sure how much is actual ppm required to be withstood. The material is going to be exposed to swimming pool water (My next question is how much chlorides is present in typical swimming pool water). The maximum temperature is ~ 185°F.
Thanks
 
Pool water usually has 2-5 ppm of active chorine. A total choride load of 50-200ppm isn't uncommon depending on the source of the water.
185F is getting tough. That is plenty hot enough for CSCC to be an issue. You probably wont see see pitting unless you get some bad biofouling or you go above ~300ppm.
Cracking will happen. You should consider the duplex alloys (2003, 2101, or 2205) for the hot section of your system. At temps below 85F 316 should do fine.

= = = = = = = = = = = = = = = = = = = =
Corrosion never sleeps, but it can be managed.
 