Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations MintJulep on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

316L base metal required suitable high temperature filler metal for GTAW & SMAW 1

Status
Not open for further replies.

nabzzban

Mechanical
Joined
Jun 4, 2014
Messages
11
Location
AE
Hi,
I submitted WPS for SS 316l with process GTAW & SMAW but client sent me back with comments, asking to find suitable filler metal for high temperature application. I went through Section IIc 5.9 and found 347 is applicable in more than 400 degree. But i don't know whether i can use 347 to weld 316l or similar base metal.Do we can use 308 ?
 
Use SFA 5.4 E316L for SMAW and SFA 5.9 Er316L for GTAW. Both match the 316L base metal.
 
thanks , but client asking for better heat resistant filler wire than 316 L.
 
No, he doesn't want that. The weld will have better creep resistance by virtue of the coarser grain size.
If you further strengthen the weld then you are likely over time to get cracking along the edges of the weld. As the base metal deforms the weld will not.
You really want them to match as close as possible in properties.
In Europe they use 316Ti, a stabilized version, but it is stronger as well.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 