Good afternoon.

I have a situation where I have to weld a 304H pipe to a P11 pipe. (D=1800mm)

I was thinking at 2 options:
1. Welding directly with ENiCrFe-3 (no PWHT, no preheat)
2. Deposit on P11 pipe an EniCrFe-3 layer (above 6mm), after that make the PWHT of the bevel and then weld the P11 buttered with 304H pipe with ENiCrFe-3.

Does anyone encounter this situation, and can tell me which can give the weld the best results.

Thank you, and have a nice day!
 
Yes, your Option 2 above based on the configuration and thickness. No preheat and no PWHT would be stretch for P11.
 
Agree, use option 2 with correct preheat and PWHT. It is far more likely to provide reliable service.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 
I also agree with the option 2 with appropriate preheat.
 