Based on your opinion and experience, can duplex stainless steels (Saf 2205) be used even slightly below 50°C as usually recommended? For example, 55 or 60°C below zero?

And for high temperature limitations is there a risk of embrittlement just already at 310°C? Or are these limits conservative?
 
I have seen pieces of good quality plate that would have good impact toughness at -55C, and that would take >5 years to develop intermetallics at 310C.
But the same is not true of fabricated items.
Once you make a weld that you cannot solution anneal and quench all bets are off.
And living with the -40C to 310C range even requires testing to verify suitability.
You should always require A923 testing for base materials and weld qualifications.
 
They can, but you are entering the realms of extremely tight quality control, and fracture mechanics. It has to be very worth it to go there.
 
The risks of low temp only apply while you are actually cold.
Though if a crack initiates then it is there.
The high temp damage is cumulative.
I did work with superferritic alloys (same mechanism).
Saw a failure after 15 years of service.
It was reaching about 370C for roughly 15min twice a day.
It adds up.
 