When detailing an uncoated weathering steel structure, are there problems associated with placing galvanized components (i.e. diaphragms, bridge drains, bolts, etc) in direct contact with the uncoated weathering steel?

I seem to think there will be some amount of galvanic action between the two components but I really can’t seem to find much guidance on this topic.

Thanks.
 
Replies continue below

Recommended for you

The two materials should be close enough electrogalvanically and there should be no additional corrosion; you might post this in the corrosion engineering forum.

Weathering steel forms a tight oxide surface and the corrosion is limited to this. As a caution, the weathered surface can drip and stain other stonework or concrete.
 
Nope, theres no problem with it. If there were, there wouldnt be any point to galvanizing anything.

It's when you start dealing with metals like copper do you have to worry.
 
They used to warn against using galvanized bolts with weathering steel girders but they don't any more.


The life of galvanized fastener coatings is only slightly reduced by coupling to weathering steel, provided the initial coating is thick enough to endure an initial period of galvanic attack prior to the development of a protective rust layer on the weathering steel.

Hg