According to literature the following steel:
BS 970 817M40 Condition 'T'
should have a final microstructure consisting of tempered marensite.
We have had a fatigue failure on a solid shaft and testing revealed the following:
Chemical properties all within specification
Mechanical Properties all within specification
Bulk hardness within specification
The mataturgist report indicated "...presence of residual bands enriched with the pressence of ferrite..."
My question is: Should this material be 100% Tempered Martensite or is there a minimum specification for % Tempered Martensite and other phases?
Thanks
Greg
BS 970 817M40 Condition 'T'
should have a final microstructure consisting of tempered marensite.
We have had a fatigue failure on a solid shaft and testing revealed the following:
Chemical properties all within specification
Mechanical Properties all within specification
Bulk hardness within specification
The mataturgist report indicated "...presence of residual bands enriched with the pressence of ferrite..."
My question is: Should this material be 100% Tempered Martensite or is there a minimum specification for % Tempered Martensite and other phases?
Thanks
Greg