Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations JStephen on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Suitable material for low temp gas stream 2

Status
Not open for further replies.

green1959

Chemical
Joined
Mar 11, 2004
Messages
21
Location
GB
I am involved in a project to design pressure equipment handling either Nitrogen, Hydrogen, Oxygen or a mixture of these - all at very low temperatures. These will all be gaseous within the equipment. Design temperature is -257C/-430F, design pressure is 20 barg.

Could someone please suggest an appropriate material of construction, bearing in mind the equipment has to be designed to a recognised design code such as ASME B31.3 or ASME VIII or similar.

Thanks in advance.
 
The pipe material that would handle this service temperature is either 304L or 316L austenitic stainless steel. The design code would be either ASME B31.1 or B31.3.
 
Additional information;
For compressor or pump pressure retaining parts or receiver tanks in this application use ASME B&PV Code, Section VIII, Div 1 design rules for low temperature service.
 
Dear metengr,

Thanks for the info. I checked ASME B31.3, Appendix A, table A-1 and saw that the minimum temperature for either 304L or 316L is stated as -425F which is just short of the -430F which I need. Do you have any further advice?

Thanks in advance.
 
green1959;

Per ASME B31.3 - 2004 Edition, section 302.2.4, paragraph h), materials that are to be used below the minimum temperature in Appendix A Table A-1 can be used provided the requirements of paragraph 323.3.2 are met.

Please review this paragraph, it is too detailed to summarize here. There should be no problems using this material if it is in a solution heat treated condition prior to service.
 
metengr,

Thank you for the excellent advice.
 
Aluminum could be used as an option . . . it might limit your fabrication options but could be cost effective
 
Meeting the impact test requirements for the welding procedure at -430F could pose a problem, especially if the Customer establishes absorbed energy limits. GTAW may be the only process acceptable for SS welding. Control of weld filler metal ferrite below 6% may be required.

 
Status
Not open for further replies.

Part and Inventory Search

Sponsor

Back
Top