Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations JAE on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Stainless steel vs. cupro-nickel exchangers

Status
Not open for further replies.

Wizeman

Mechanical
Joined
Oct 11, 2007
Messages
16
Location
CA
Hi all,

I'm wondering if anyone has had long-time experience with stainless steel exchangers on open-loop geothermal systems.

The reason I am asking is because the heat pumps with stainless steel exchangers are slightly less expensive (and more readily available where I am) than cupro-nickel exchangers.

So to re-iterate: is it OK to use a stainless steel exchanger in a water-source heat pump on an open ground loop?

Thanks,

-Vince
 
does the water have chlorides?



Patricia Lougheed

Please see FAQ731-376: Eng-Tips.com Forum Policies for tips on how to make the best use of the Eng-Tips Forums.
 
I honestly don't know. I will have to ask.
 
Reason I'm asking is that presence of chlorides (which tend to be common in open loop water systems) cause SS to develop stress corrosion cracking -- which means replacement. A copper-nickel heat exchanger might be more expensive up front, but might last longer. You may need to do a cost comparison to decide which is your better option.

Patricia Lougheed

Please see FAQ731-376: Eng-Tips.com Forum Policies for tips on how to make the best use of the Eng-Tips Forums.
 
The main factors in the preliminary selection of the heat exchanger (HE) materials are: physical properties, mechanical properties, corrosion resistance, fabrication and joining technology, experience, availability and cost. Thermal conductivity of the fin material has a direct effect on heat transfer efficiency, the higher the better.

Usually air-side heat transfer characteristics of fin-and-tube heat exchangers are determined from limited experimental data. But the overall heat transfer coefficient Uh is proportional to the tube and fin thermal conductivity. Changing the materials to a less conductive alloy will affect the system performance.

Stainless steel 316 (most commom HE) can exhibit stress corrosion cracking above about 60°C and is considered resistant to potable water with up to about 1000mg/L chlorides at ambient temperatures, reducing to about 500mg/L at 60°C.
 
Thanks boo1,

So basically if the well water doesn't go above 45 F (7.2 C) year-round and the chlorides stay below 1000mg/L I will be fine with Stainless steel?

Makes sense.

-Vincent
 
Analysis should shows you if the HE will perform within the required heat regection.
 
Do a chemical analysis of the liquids on both sides of the HX.

It's money well spent.

Copper nickle systems are good at chloride resistance, but you better not have any traces of ammonia in the system.

Be specific with your materials ......

Which particular cupro-nickle alloy are you considering ?

What is the temperature range of service ????

-MJC

 
VPL asked about chlorides; I'll ask about H2S. H2S is not uncommon around geothermal plants, in fact it is prevalent. Cu-Ni doesn't like H2S.