Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Spring back rates for 316 SS 1

Status
Not open for further replies.

rsmichaud

Mechanical
Mar 1, 2005
2
Does anyone have any data on spring back rates for 316 SS? I am trying to bend plates (approx 8" x 5" x 0.25") and in order to size the die correctly, I would like to factor in the spring back rate.
 
Replies continue below

Recommended for you

You need to know the bend radius, and condition of the material. Using the information in ASM Handbook, Vol 14,

Bend radii, degree springback in a 90 degree bend

304 ss
1t 2 degrees
6t 4 degrees
20t 15 degrees


Also, springback is approximately proportional to the equation below;

(0.2YS + UTS)/2.


 