My application does not involve elevated temperatures.
I would like to process the termination ends of Kanthal or Alloy-875 resistance wire to make it solderable with standard electronic solders.

I understand that Nichrome wire can be tinned using Steel solder flux with standard
solder provided that the acid flux is removed after tinning.
Nichrome-A – 80% Ni, 20% Cr
Nichrome-C - 61% Ni, 15% Cr, balance Fe

I would like to do something similar with Kanthal or Alloy-875 if possible.
Alloy 875 - 22.5% Cr, 5.5% Al, 5% Si, 1% C, balance Fe
Kanthal-A – 22.5% Cr, 5.3% Al, 0.7% Si, 0.08% C, 0.5% Mn Balance F3


Does anyone have application experience along these lines that they could share?

Thank you,
Erro11


 
Replies continue below

Recommended for you

I've tinned fairly large pieces of 304 stainless using a torch to heat the metal, then brushing on zinc chloride/zinc fluoride flux. As you say, follow this with a good washing in an alkaline cleaner, rinse, maybe a little work with a Scotchbrite pad. Should work for any chrome/nickel alloy.
 
How about a tinning with silver solder, after that regular solder would stick.
 
Before silver solder will "stick" to the chrome-containing alloys, you will still need to use a fairly agressive, acid flux. Something with fluorides, or fluoro-borate compounds, that will etch the chrome oxide.

For wire, a quick method is to heat the wire and dip into the flux bottle. But it's also a good way to crud up your flux.

You may find you need to do several heat/flux/wash/buff cycles before you get a smooth, evenly tinned surface.
 