Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations KootK on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

Sec I fillet contour 1

Status
Not open for further replies.

fazel1

Industrial
May 7, 2005
69
in ASME SecI , PW-36.2 refer the quality of fillet weld contour to ASME SecIX, but I couldn't find anything about this in SecIX. could anybody please help me.
 
Replies continue below

Recommended for you

In Section I of the 2001 Edition/2003 Addendum of the ASME B&PV Code, PW-36.2 makes no reference to Section IX. The paragraph is titled "Fillet Welds". It mentions adequate penetration, maximum undercut and the surface of fillet welds with no specific reference to Section IX..

No mention in the 2004 addition of Section I.

 
would you please kindly tell me the maximum amount of undercut and the requirement for surface of fillet weld base on ASME 2003 addendum?
 
Maximum undercut;
1/32" OR 10% of wall thickness, whichever is the lesser value.

Contour;
No coarse ripples or grooves, smooth transition. Concavity of the weld face is permitted provided it does not encroach on the required weld thickness.
 
is there any convexity permitted?
 
Yes. However, the convexity must not exceed maximum reinforcement or result in abrupt transitions or excessive undercut with the base metal.
 