Good Day Experts,

I am preparing a Procedure Qualification Record for the combination of GMAW-short circuiting and GTAW process.
GTAW - for root pass for the maximum of 5.0mm
GMAW - for 2nd pass to copping.
My test coupon (tube) thickness is 8.9mm

My Question is - is this possible for the combination the 2 processes?
- how can I compute and balance the weld metal thickness range of the 2 processes?
since the short circuiting requirement - less than 13mm (x1.1 of the base metal and weld metal)
and for the GTAW is x2 of the weld metal and base metal.
how can I balance the weld metal thickness range and weld metal thickness range?

thanks in advance mga sir.
god bless!

Best Regards,
Mark Chester

 
Dear Mark,

Go for 4 mm by GTAW and rest by GMAW.

So, in the WPS, you can go upto 8 mm by GTAW and then upto 10 mm by GMAW.

You will be below 19 mm so need not include PWHT in the PQR.

Regards.

DHURJATI SEN
 
BM Qualified is limited to 1.1 x Coupon thickness, even when multi-process: It get's a little more tricky when dealing with weld metal qualified....using the max basemetal qualified of 9.79mm (1.1x8.9mm), you could have anywhere from 5.5mm to 9.79mm of GTAW, and 0 - 4.29mm GMAW-S, and any combination in between. How you get the welder to understand this is up to you.

BPV Section IX
Edition/Addenda:
Para./Fig./Table No:
Subject Description: Section IX, QW-403.10, Short-Circuiting Mode
Date Issued: 09/24/1996
Record Number: BC96-001
Interpretation Number : IX-95-33
Question(s) and Reply(ies):
Question: Does QW-403.10 limit the base metal thickness qualified to 1.1T for a combination GMAW-S/SMAW PQR test coupon thickness "T" less than ½ in. when used to support a combination GMAW-S/SMAW WPS?

Reply: Yes.
 