HI experts ,
I have a problem with pmma part , that is about some "Air trap" , some are inside and some are at surface and I preheat the resin perfectly ,
now how Should I adjust setting such as : Speed , press and time of Injection ,charging ......

Thanks
 
Replies continue below

Recommended for you

Is the material dry.

Are you sure it is air trap and not contraction void.

Without seeing the part and fault, I will take a SWAG at it just for fun.

Try injecting fairly slow with a fairly warm mould, use as much pressure as you can without causing flash. Make sure the gate and runner are big enough.

Hold up injection pressure until you get no more weight gain from extra time.

Regards

eng-tips, by professional engineers for professional engineers
Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Oh

And read the troubleshooting guides that come with the machine and will be provide on request from the raw materials supplier.

Regards

eng-tips, by professional engineers for professional engineers
Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor