PCTFE - Amorphous / Crystalline

Status
Not open for further replies.

PeterIgg

Petroleum
Apr 6, 2003
99
Is anyone aware of a test that can be performed to give a reliable indication as to whether the form of the material is in either the crystalline or amorphous state?

We use this material for seals in cryogenic applications and experienced a failure when using the crystalline form of the material as opposed to the amorphous (or 'more amorphous') grade.

Can anyone direct me to any useful information on this product - our suppliers have been as helpful as possible but, obviously, need to protect their proprietary processes.
 
Replies continue below

Recommended for you

Specific gravity can often be used if the material is unfilled, the higher the SG, the greater the crystalinity in most cases. Water and ice being a notable exception.

Regards
pat pprimmer@acay.com.au
eng-tips, by professional engineers for professional engineers
Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Testing for strength vs temp should reveal crystalline vs amorphous properties. The crystalline material will exhibit more strength, but the amorphous material will exhibit more energy absorption: the area under the stress-strain curve.

In a gearbox that experienced stall at travel limits in the mechanism, we had trouble with crystalline Acetal gears, but the problem went away when we switched to Nylon 6.
 
X-ray diffraction is the method used to determine crystallinity directly . The other methods are indirect, though much less complicated and much less expensive.

Regards,

Cory

Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Cory

Even some polymer manufacturers do not have in house access to X-ray diffraction, however i agree it is the only "real method".

Regards
pat pprimmer@acay.com.au
eng-tips, by professional engineers for professional engineers
Please see FAQ731-376 for tips on how to make the best use of Eng-Tips Fora.
 
Guys

Thank you all for your comments - much appreciated.
 
Differential Scanning Calorimetry is a very simple way to determine if your polymer is crystalline or amorphous.
 