Here under is the surface preparation recommended by Total in GS EP COR 350
Stainless steels shall be segregated, carbon steel supports for storage shall be systematicallypainted, and lifting equipment shall prevent iron contamination.
Stainless steel surfaces to be coated shall be etched or degreased and blast-cleaned with a
non-ferrous and chlorine-free abrasive.
The blast cleaning procedure to be submitted to Company shall include:
• Abrasive composition to obtain a surface roughness of Ra = 10 microns (8 microns
acceptable locally)
• Dust level (maximum level 2 maximum according to ISO 8502-3)
• Substrate contamination checks. Ferrous contamination/direct colorimetry method using
Prussian blue (potassium ferricyanide) - No surface pollution is acceptable