Hello
I'm having problems to get MBB standard like DBL 5563-21 just in elongation at break like the results below:
1000h@100°C ageing in air
change in Hardness (+18 Shore A max) - +16 Shore A
Tensile at break (7 MPa min) - 13,5 MPa
Change in tensile (30% max) - -7,3%
Elongation at break (160 % min) - 120%
Change in elongation (50 % max) - -62,4%
This is the compound formulation i'm already using:
NBR with medium ACN - 100
ZnO - 4,0
Stearic Acid - 1,5
Antiozonant Wax - 2,0
IPPD - 2,0
TMQ - 1,0
ZMTI - 2,0
Carbon black N762 - 52
Carbon black N330 - 10
TP 759 plasticizer - 4,0
Sulphur - 0,3
TMTD - 1,0
CBS - 2,0
ZDBC - 1,5
DTDM - 2,2
WB 16 - 2,0
the MBB normally tests the final part laminated too and this is a problem.
If anybody can help me i will appreciate so much.
Thanks in advance
I'm having problems to get MBB standard like DBL 5563-21 just in elongation at break like the results below:
1000h@100°C ageing in air
change in Hardness (+18 Shore A max) - +16 Shore A
Tensile at break (7 MPa min) - 13,5 MPa
Change in tensile (30% max) - -7,3%
Elongation at break (160 % min) - 120%
Change in elongation (50 % max) - -62,4%
This is the compound formulation i'm already using:
NBR with medium ACN - 100
ZnO - 4,0
Stearic Acid - 1,5
Antiozonant Wax - 2,0
IPPD - 2,0
TMQ - 1,0
ZMTI - 2,0
Carbon black N762 - 52
Carbon black N330 - 10
TP 759 plasticizer - 4,0
Sulphur - 0,3
TMTD - 1,0
CBS - 2,0
ZDBC - 1,5
DTDM - 2,2
WB 16 - 2,0
the MBB normally tests the final part laminated too and this is a problem.
If anybody can help me i will appreciate so much.
Thanks in advance