What's the material and finish for the black spring metal in this picture?

I am designing a spring and I want it to be flex and hard as this metal?

How should I specify in my drawing?

stock-photo-large-black-paper-clip-isolated-on-white-62572585.jpg
 
Replies continue below

Recommended for you

Thanks for replying.

I was prompted by a vendor, but I am not sure if this is True.
He said that material is Manganese - Steel.

Does anybody here have any idea what material could this clip be made of?
And also, could it be pre heatreated or Post heat treated in real production?

Thanks
C1
 
Thanks goahead. So on my drawing notes I should probably provide information about :

1. Use spring steel (any specific ?)
2. Anneal before forming
3. Harden and temper after forming ( what temp / hrc ?)

Can anybody provide more info.
Thanks
C1
 
caddone,

Here is an example of a proper specification for this type of part:

Material: ASTM A684, 1050-1074 spheroidized annealed
Treatment: Austemper to 44-51 HRC
Coating: black electrocoat, thickness 10 μm minimum

Another option for the coating is black oxide. This can specified according to ISO 11408, DIN 50938, SAE AMS 2485, or MIL-DTL-13924.
 
Goathead - some spring steels are not annealed. Helical compression springs made from 304L wire are common, and they are definitely not annealed, though they may be stress-relieved after forming. But the strength of those springs is dependent upon the fact that the wire began with a yield strength of about 25 ksi and ended as a wire with a yield strength of up to 250 ksi, then it's wound into a spring.

Doug
 
Anodized aluminum, 6061 T6 sheet metal.

Regards,
Cockroach
 
Cockroach - I haven't heard how a AL 6061 be used for a spring.
 
Could be an alloy, pure guess. Why not google "What is a paper clip made of" and doing some basic research? Might be better than guessing, no?

Regards,
Cockroach
 
The result from a google search had various kinds of spring steel.
In fact the answer from TVP (above) gave me all the information I needed. But was curious about AL you mentioned.

But I agree, It might be an alloy, if its AL.
 