I'm looking for a recommendation for a material to be used for soldering fixture. Material needs to have low thermal conductivity, ba able to withstand the heat and be machinable.
 
Replies continue below

Recommended for you

Corning MACOR machinable ceramic.
I think McMaster carries it and similar stuff from Cotronics.


Mike Halloran
Pembroke Pines, FL, USA
 
Macor is a resonable choice k = 1.5 W/m-K. The green, machinable stuff will pickup solder flux and wet to solder over time, better results if you bake it out after machining.

Fused (sintered) amorphous boron nitride can be k = 3 W/m-K. Machines well with abrasive tools, though it's a bit brittle and weak, but it has lovely non-stick properties for braze/solder tooling. You can buy it in rods and plates from McMaster-Carr, amongst other sources.

Foamed silica (Space Shuttle heat shield tile material) is one of the lowest conductivity materials around ( k = .19 W/m-K. This stuff too is brittle and weak, but can be machined easily with abrasive bits (heck, with a pocketknife too). Also very low wettability to molten metals, fluxes, etc.
 