dieselofdog

Materials
Joined
Feb 11, 2014
Messages
28
Location
AU
Hi,

I have a casting made to ASTM A890 1A, Duplex Stainless. The casting has failed hydro testing, a weld repair has been made. I know Solution annealing is required. The question has been raised to conduct a workshop localised PWHT, heating to above 1100 deg C followed by quenching (buckets of water and wet rags).

I am concerned that potentially more damage could be done as there is a chance of forming embrittled precipitates in the surrounding region. I believe the entire casting should be uniforming heated and quenched.

Am I on the right path?
 
Yes, local solution heat treatment is NOT recommended.
 
Even though this alloy is less sensitive than some of the other duplex grades, you are correct.
The entire casting should be re-annealed and quenched.
Make sure that the quench tank is large enough to to assure adequate cooling.

= = = = = = = = = = = = = = = = = = = =
P.E. Metallurgy, Plymouth Tube
 