Tek-Tips is the largest IT community on the Internet today!

Members share and learn making Tek-Tips Forums the best source of peer-reviewed technical information on the Internet!

  • Congratulations JStephen on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

INCOLOY 800HT 3

Status
Not open for further replies.

gguerrageci

Mechanical
Joined
Dec 16, 2005
Messages
9
Location
MX
i WOULD LIKE TO KNOW THE MAXIMUM OPERATION TEMPERATURE FOR A PIPE OF INCOLOY 800HT
 
Look for ASTM B408, ASME SB-408 or UNS N08800. The Young's modulus and S Stress values are published with suitable numbers to about 1100 degree F in Various ASME B31.1, B31.3, "Physical and Mechanical Properties". The ASME Boiler and Pressure Vessel Code, Section II Materials, Part D - Properties - S values avalance down from 13000 psi at 1100 deg F to 2000 psi at 1300 deg F. Thus, I would avoid N08800 above 1100 degree F.



John
 
See below for specific information on Incoloy 800;



Suggest Incoloy 800 HT pipe/tube under ASME B 407.

Maximum service temperature depends on the application. For example, Section I (boiler application) the maximum service temperature is 1500 deg F, where Section VIII, Div 1 application is 1650 deg F for unfired pressure vessels.

For B31 Pressure Piping (B31.1 - Power Piping) maximum service temperature is 1200 deg F. For B31.3 (Process Piping), the maximum service temperature is 1650 deg F.
 
Metengr,

The website link you provided has excellent information on it. Do you, or anyone else, know of a website with similar information for ferrous alloys, namely various grades of steel. I have found the following website to be helpful.


Can someone recommend another website? Thank you all!
 
Do any know the allowable stress for 1500°F to 1650°F for incoloy 800HT
 
Yes, per ASME B&PV Code, Section II, Part D, for UNS
08811, Incoloy 800HT

1500 deg F 2.2 Ksi
1550 deg F 1.6 Ksi
1600 deg F 1.2 Ksi
1650 deg F 0.91 Ksi


 
This allowable stresses aplyy to ASME B31.3 ?
 
No. For B31.3

1500 deg F 1.9 Ksi
1550 1.5
1600 1.2
1650 1.0

 