Hi all,

We have a small 316 SS tank that we use for passivating small stainless components with a 50/50 mix of water and Nitric acid 42BE.

A new employee changed out the tank last night and added Hydrochloric acid to the water instead of Nitric acid. By time the acid was pumped out, it had etched/pitted the tank.

It doesn’t appear that any of the pitting is too deep, and this is probably a stupid question, but can we still use the tank for Nitric acid?

I wasn’t sure if the stainless tank had some sort of protective layer that the hydrochloric has eaten away leaving it unsuitable for our passivation process.

Thanks for your help!
 
You should be able to re-passify the surface, nitric acid should be effective for re-passivation.
 
As stated above the reintroduction of HNO3 after a through rinsing will passivate the tank in progress. The surface will be very sensitized after the exposure to HCl so you may get a little rust which need s to be removed before any production parts are introduced into the bath.

If you do please post.
 
Stainless steel resistance to corrosion rely on a superficial passive layer.. in an oxidant solution, like nitric acid, the passive layer is restored..
have a look at this page of BSSA for Nitric Acid passivation:

also



s


Corrosion Prevention & Corrosion Control
 
Thank you for the input everyone. And the passivation website was very informative.

Kim
 
If some areas have been roughened a lot you may need to go in with mechanical polishing and smooth them out some. If it is too rough it could catch debris and cause marking/streaking issues.

= = = = = = = = = = = = = = = = = = = =
Plymouth Tube
 
The reason for special attention on the welds is that the fabrication welds will have a residual ferrite in them. and that ferrite is attacked very quickly in HCl.
If you saw roughening of the base metal you may have lost a significant amount of metal out of the welds.

= = = = = = = = = = = = = = = = = = = =