Continue to Site

Eng-Tips is the largest engineering community on the Internet

Intelligent Work Forums for Engineering Professionals

  • Congratulations waross on being selected by the Eng-Tips community for having the most helpful posts in the forums last week. Way to Go!

High temp data for SA 387 Gr.22 Cl.2

Status
Not open for further replies.

bagnamento

Nuclear
Feb 23, 2005
30
Hi everybody,
I need tensile properties (yield point 0.2% and ultimate tensile strength) data for ASME SA 387 Gr.22 Cl.2 (21/4Cr, 1Mo) steel.
In particular I need experimental data (not ASME II-D design data) for temperatures within 840-1110°F (450-600°C).

Thanks
 
Replies continue below

Recommended for you

bagnamento;
I found some information that might be of help to you. The elevated temperature mechanical property data is for 2.25% Cr - 1%Mo alloy steel from the following publication "Report on The Elevated Temperature Properties of Chromium-Molybdenum Alloy Steels" compiled by ASTM-ASME Joint Committee on the Effect of Temperature on the Properties of Metals, Tech Pub 151.

The data below pertains to bar. Despite the different product grade, it will at least give you a ballpark estimate on properties - deg F, Ksi

Temp YS (0.2%) UTS
900 F 38.25 63.75
1000 F 35.75 49.75
1100 F 34.25 39.10
 