Hello, I have this elliptical head 2:1, cold formed from plate, with forming strain=6,2% acc. to ASME VIII Div.I UG-79 formula and deformation F=28,52% acc. to EN 13445-4 9.2-1.
Applicable construction code is EN 13445.
Head is not for lethal service and starting thickness is 12mm.
Material: ASTM SA/A 516 Gr.70N
Question: does the head need to be heat treated or not? tnks
 
Replies continue below

Recommended for you

It's GR.70N so already heat treated?

GR.70 = P355GH (EN 13445-2, Table E.2-1, plate and strip - material group 1.2)

9.4-1 in EN 13445-4
Material group 1.2, If F > 5%, yes to heat treatment
Thermo mechanically treated steel note does not apply

 
Gr.70N is supplied normalized. So is HT still necessary? Even if from plate?
 

Caloooomi, I've just read par.8 of EN, but my head is COLD formed from plate. "Hot forming" of 9.3.2 in EN refers to this phase I think, not to the treatment of the plate itself. Or not?
 
Sorry, my fault! I have a wrong version of EN with missing pages...
Ok, table 9.4-1 is clear: thank you!
 