We have a strange request to etch a gold structure. The gentleman claimed he had a company use an etchant that contained cyanide. I don't have this in house and don't plan on ordering it. Is there any quality alternative you can recommend?
 
Replies continue below

Recommended for you

You may try to use potassiumferricyanide, it may work, too.
I know it dissolves Ag -- I don't know about speed...


<nbucska@pcperipherals.com>
 
The first on is the one I've used. This is essentially Aqua-Regia tones down. The etchant is really nitrosyl chloride. Do this in a hood or outside and stay up wind.
I threw in the cyanide one just for you.


Material: Gold (Au), platinum (Pt), palladium (Pd)
Type: Macroetching
Method: Chemical etching
Etchant (electrolyte): 66 ml hydrochloric acid, 34 ml nitric acid.
Procedure: Few minutes. Use hot and fresh!.
Remarks: Au, Pt alloys and Pd alloys.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 43.

Material: Pure gold (Au), palladium (Pd) and rhodium (Rh)
Type: Microetching
Method: Chemical etching
Etchant (electrolyte): 40 (1) ml nitric acid, 60 (10) ml hydrochloric acid.
Procedure: Few seconds to 1 min. May require heating. Use only fresh!.
Remarks: Pure Au and Pd. Au-Pd, Pd alloys with more than 90 % concentration of precious metals. Rh alloys.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p.44.

Material: Palladium (Pd), gold (Au) and platinum (Pt)
Type: MicroetchingMethod: Chemical etching
Etchant (electrolyte): 100 ml distilled water, 10 g potassium cyanide.
Procedure: 30 s to 2 min.
Remarks: Au alloys with less thn 90 % content of precious metals.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.

Material: Palladium (Pd), gold (Au) and platinum (Pt)
Type:: Microetching
Method: Chemical etching
Etchant (electrolyte): 100 ml distilled water, 10 g ammonium persulfate.
Procedure: 30 s to 2 min.
Remarks: For Au alloys with high content of precious metals. White gold. Pd and Pt alloys.
Reference: G.Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.

Material: Gold (Au), palladium (Pd), platinum (Pt)
Type: Microetching
Method: Chemical etching
Etchant (electrolyte): 30 (50) ml distilled water, 25 (100) ml hydrochloric acid, 5 (10) ml nitric acid.
Procedure: 1-5 min. Use hot.!. Remove precipitate of gold chloride with ammonia water.
Remarks: Pure Pt and Pd. Au alloys. Proportions in parentheses especially useful for Pt.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.

Material: Gold (Au), palladium (Pd), platinum (Pt)
Type: Microetching
Method: Chemical etching
Etchant (electrolyte): 100 ml hydrochloric acid, 1-5 g chromium (VI) oxide.
Procedure: Seconds to minutes.
Remarks: Pure Au and Au-rich alloys. Pd and Pd alloys.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.

Material: Gold (Au), palladium (Pd), platinum (Pt)
Type: Microetching
Method: Chemical etching
Etchant (electrolyte): 30 (50) ml distilled water, 25 (100) ml hydrochloric acid, 5 (10) ml nitric acid.
Procedure: 1-5 min. Use hot.!. Remove precipitate of gold chloride with ammonia water.
Remarks: Pure Pt and Pd. Au alloys. Proportions in parentheses especially useful for Pt.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.

Material: Gold (Au), palladium (Pd), platinum (Pt)
Type: Microetching
Method: Chemical etching
Etchant (electrolyte): 100 ml hydrochloric acid, 1-5 g chromium (VI) oxide.
Procedure: Seconds to minutes.
Remarks: Pure Au and Au-rich alloys. Pd and Pd alloys.Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.


Material: Platinum (Pt), gold (Au)
Type: Microetching
Method: Electrolytic etching
Etchant (electrolyte): 100 ml distilled water, 5 g potassium cyanide.
Procedure: 1- 2 min, 1-5 V ac, 0.5-1.5 A/cm2, Pt cathode.
Remarks: Pt and Pt alloys, Au and Au alloys.
Reference: G. Petzow, Metallographic Etching, ASM (American Society for Metals), 1978, p. 45.
 
Thanks Unclesyd. You gave me some options. I will try them now.


Yeah I can't make any of the ones that stink too bad. I made that mistake last Wed (HCL and H202). I had it in the fume hood, but didn't have the exhaust on. Big mistake. All I can say is the last half hour of work in the lab was cancelled!

 