I have successfully welded cupronickel(90:10) with matching consumables. However, there are two reasons put forward for using 70/30 as the weldmetal for the material. The first is that considerable coring can occur in the 90/10 weldmetal thus giving denuded regions which corrode preferentially. The second is that the specification for the parent and weldmetal for 90/10 is the same. Therefore you may get parent with max nickel and weldmetal with min nickel making the weldmetal anodic. To overcome both potential problems CuNi 70/30 weldmetal is used. SFA 5.7, ERCuNi is CuNi 70/30