Can any one tell me the modern equivelent of steel EN 3 and EN 8 These are from superceeded european system
 
Replies continue below

Recommended for you

Bogues

Go to and go to the library section. Their Orange Handbook contains a section at the back with a cross reference from all the old EN numbers to their modern equivalents.

They say that EN3 is equivalent to 055M15, and that 070M20 is nearer to EN3A.

Bruv
 
Thanks a lot guys Ive now stopped pulling my hair out!
 
This is probably splitting hairs, but I do not agree that 055M15 is equivalent to the old EN3 grade. The new 070M20 is obviously identical to EN3A, but I still think this is a better equivalent based on the C & Mn content:

EN3 0.25 max C 1.0 max Mn

EN3A 0.16-0.24 C 0.50-0.90 Mn

070M20 0.16-0.24 C 0.50-0.90 Mn

055M15 0.20 max C 0.80 max Mn

Anyway, it sounds like you found what you needed. Good luck.

 