Coudl some one tell me if WCC and WCB variations of A216 are equal? I have a customer that is requesting WCC materials, and my supplier is offering WCB for my pressure releif vlave offering!

Bruce
 
Replies continue below

Recommended for you

The two grades are similar but not identical. Here is a summary of the differences:

WCB has 0.30% max C concentration, 1.00% max Mn concentration, and 36 ksi/250 MPa yield strength.

WCC has 0.25% max C concentration, 1.20% max Mn concentration, and 40 ksi/275 MPa yield strength.
 
A quick addition is that when WCB is required WCC is always an acceptable alternative but unfortunatley not the other way round. The properties of WCC are superior to WCB.
 