Hi Guys,
I am wondering if you can help me specify a riser clamp neoprene liner that would work effectively in marine environment.
 
Replies continue below

Recommended for you

Many thanks Steve appreciate it,

I checked it out and seems great yet I am still wondering if the same compression set requirements apply to the clamp liners?

Any thoughts about the acceptance criteria for seawater absorption & ozone resistance for such application?
 
Seawater absorption:
- Max 5% volume change
- Reduction in tensile strength max 15%
- Change in hardness max +5/-5 units
- No cracking, crazing, blistering or splitting after immersion

Ozone resistance:
- No cracking or 'other detrimental effects'

Steve Jones
Materials & Corrosion Engineer
 
Thanks Steve, actualy thanks twice for the two replies :)

much appreciate the expert advice
 