Dear experts,

What is the advantage of normalizing on a steel plate ?

Let say I have plate 30 mm A516 Gr. 60 normalized and A516 Gr.60 without normalized.

What is the different ? Better tensile strength ? Better toughness ?

Syah
 
Replies continue below

Recommended for you

Yes, normalizing improves through thickness tensile properties and notch toughness is improved.
 
Everything is better with normalization, except possibly cost.
In ASTM A516, normalizing is mandatory for all grades over 1½" thick; however it is mandatory for thickness less than 1½" if notch toughness is required.
Realistically, your buyer will probably return with Grade 70, either dual certified or because it is more available.

"Everyone is entitled to their own opinions, but they are not entitled to their own facts."
 