The quick breakdown:
- 52100 Steel, through-hardened to a martensitic phase for bearings.
- Material from other sources with this part # are running fine, but this specific batch of material is growing/shrinking all over the place, going way out of round and out of flat.
- Cut and polished a sample, Nital Etched (5%) and here's what it looks like at 150x:
Doesn't look like the normal spiky pine-needles of martensite, that's for sure. I'm thinking that perhaps the dark areas are oversized spheres of Pearlite that didn't fully dissolve, but I'd love some other input. (Never was good at microstructures.)
For the record: It's cheap-ass Chinese Steel with questionable carbon smudges on the mill certification.
- 52100 Steel, through-hardened to a martensitic phase for bearings.
- Material from other sources with this part # are running fine, but this specific batch of material is growing/shrinking all over the place, going way out of round and out of flat.
- Cut and polished a sample, Nital Etched (5%) and here's what it looks like at 150x:
Doesn't look like the normal spiky pine-needles of martensite, that's for sure. I'm thinking that perhaps the dark areas are oversized spheres of Pearlite that didn't fully dissolve, but I'd love some other input. (Never was good at microstructures.)
For the record: It's cheap-ass Chinese Steel with questionable carbon smudges on the mill certification.