Is 316 SS, susceptible to pitting/crevice corrosion in stagnant groundwater at less than 30 deg C. with chloride in the range of 2000 ppm. Also possibility of MIC (SRB) corrosion in swampy.
 
Replies continue below

Recommended for you

I think MIC will be your worst enemy based on my experience.

You will eventually get pitting at the ground air interface. From what I've seen pitting isn't really a big problem as the pits are very shallow. The only thing you will notice is the pipe will be a little rusty.
 
a "safe" limit of chloride concentration for SS 316 in water is set to approx 1000-2000 ppm. This limit is a function of several factors like:
-possibility of crevice conditions
-possibility of evaporation and concentration of chlorides
-condition of the exposure, fluid velocity; stagnant water will cause the steel to become active if no oxygen will reach the steel surface
-composition of the weater and possibility of MIC
-temperature..

In my opinion in your conditions you'll have the possibility of either pitting and crevice.
The acceptable limit of chloride is also a function of the criticality of your service.

Stainless Steel Corrosion

GUIDELINES FOR SELECTION OF NICKEL STAINLESS STEELS FOR MARINE ENVIRONMENTS, NATURAL WATERS AND BRINES (1987) (pub. 1987)


S.

Metal Corrosion
 
Status
Not open for further replies.

Part and Inventory Search

Sponsor