Equivalent to 16MnCr5 to sae steel
Equivalent to 16MnCr5 to sae steel
(OP)
This steel has
C: 0.14 to 0.19
Si: 0.40 max
Mn: 1.00 to 1.30
Cr: 0.80 to 1.10
How near is from Sae 8620 or SAE 3115?
C: 0.14 to 0.19
Si: 0.40 max
Mn: 1.00 to 1.30
Cr: 0.80 to 1.10
How near is from Sae 8620 or SAE 3115?
Pardal





RE: Equivalent to 16MnCr5 to sae steel
8620 3115 5115
C 0.18/0.23 0.13/0.18 0.13/0.18
Mn 0.70/0.90 0.40/0.60 0.70/0.90
Si 0.15/0.35 0.20/0.35 0.15/0.35
P 0.030 max 0.040 max 0.030 max
S 0.040 max 0.040 max 0.040 max
Cr 0.40/0.60 0.55/0.75 0.70/0.90
Ni 0.40/0.70 1.10/1.40 0.70/0.90
Mo 0.15/0.25 - -
RE: Equivalent to 16MnCr5 to sae steel
Sorry I can not mark your post as helful because I can not open the java script.
Thank again
Pardal