INTELLIGENT WORK FORUMS
FOR ENGINEERING PROFESSIONALS

Log In

Come Join Us!

Are you an
Engineering professional?
Join Eng-Tips Forums!
  • Talk With Other Members
  • Be Notified Of Responses
    To Your Posts
  • Keyword Search
  • One-Click Access To Your
    Favorite Forums
  • Automated Signatures
    On Your Posts
  • Best Of All, It's Free!
  • Students Click Here

*Eng-Tips's functionality depends on members receiving e-mail. By joining you are opting in to receive e-mail.

Posting Guidelines

Promoting, selling, recruiting, coursework and thesis posting is forbidden.

Students Click Here

Jobs

Appropriate Neoprene liner for offshore riser clamps

Appropriate Neoprene liner for offshore riser clamps

Appropriate Neoprene liner for offshore riser clamps

(OP)
Hi Guys,
I am wondering if you can help me specify a riser clamp neoprene liner that would work effectively in marine environment.

RE: Appropriate Neoprene liner for offshore riser clamps

(OP)
Many thanks Steve appreciate it,

I checked it out and seems great yet I am still wondering if the same compression set requirements apply to the clamp liners?

Any thoughts about the acceptance criteria for seawater absorption & ozone resistance for such application?

RE: Appropriate Neoprene liner for offshore riser clamps

Seawater absorption:  
- Max 5% volume change
- Reduction in tensile strength max 15%
- Change in hardness max +5/-5 units
- No cracking, crazing, blistering or splitting after immersion

Ozone resistance:
- No cracking or 'other detrimental effects'

Steve Jones
Materials & Corrosion Engineer
http://www.oilandgaspeople.com/cv/11499664
http://www.linkedin.com/pub/8/83b/b04
 

RE: Appropriate Neoprene liner for offshore riser clamps

(OP)
Thanks Steve, actualy thanks twice for the two replies smile

much appreciate the expert advice
 

Red Flag This Post

Please let us know here why this post is inappropriate. Reasons such as off-topic, duplicates, flames, illegal, vulgar, or students posting their homework.

Red Flag Submitted

Thank you for helping keep Eng-Tips Forums free from inappropriate posts.
The Eng-Tips staff will check this out and take appropriate action.

Reply To This Thread

Posting in the Eng-Tips forums is a member-only feature.

Click Here to join Eng-Tips and talk with other members!


Resources